Nickel Release Testing: EN 12472:2020 + EN 1811:2023
Nickel release is measured, not asserted. For a coated piece the sequence is EN 12472:2020 wear-and-corrosion pre-treatment first, then EN 1811:2023 measurement, then comparison against the REACH Annex XVII entry 27 limits: below 0.2 µg/cm²/week for post assemblies and below 0.5 for other prolonged skin contact.
Nickel release
Not detected — below 0.05 µg/cm²/week
Tested to EN 12472:2020 & EN 1811:2023, the wear-and-corrosion pre-treatment first, then a week in artificial sweat and measurement of what released. REACH Annex XVII entry 27 sets below 0.2 µg/cm²/week for post assemblies inserted into pierced ears or other pierced body parts. Coated items fall under entry 27(c), which requires the limit to hold throughout at least two years of normal use. That is what the pre-treatment step simulates, and why a report without it tells you very little about a coated item.
Why it matters
Nickel sensitivity is not evenly distributed
For a line aimed at women, and especially one built around earrings, nickel release is the most likely single cause of returns and complaints.
What the research measured
The EDEN study screened a general population sample across five European countries (n = 3,110) for contact allergy. Nickel sensitization was found in 22.2% of women and 5.2% of men, women roughly 4.3 times as often. Among people with three or more piercings the figure was 27.6%.
We report this as a sourced finding about a population, not as advice about anyone's skin and not as a claim about what a product will do.
What it means for a purchase decision
Earrings are the largest category in a women's assortment and ear posts are the strictest exposure case in the regulation. A supplier who cannot produce a properly sequenced report on this one point is asking you to carry the risk on the category most likely to generate it.
That is the whole argument for this page: not that our pieces are safe for everyone, but that the question has an answer and the answer is documented.
The limits
REACH Annex XVII entry 27 has three tiers, not two
The third tier governs every plated piece we make.
| Paragraph | Item category | Limit | Additional requirement |
|---|---|---|---|
| (a) | Post assemblies inserted into pierced ears or other pierced body parts | below 0.2 µg/cm²/week | — |
| (b) | Other articles intended for direct and prolonged contact with the skin | below 0.5 µg/cm²/week | — |
| (c) | Articles under (b) that carry a non-nickel coating | below 0.5 µg/cm²/week | The limit must hold throughout at least two years of normal use |
Method
The sequence, and why it cannot be reordered
For a coated item the three steps below run in this order. An uncoated item is assessed as supplied, under paragraph (a) or (b), so the first step does not apply to it.
EN 12472:2020, wear and corrosion pre-treatment
An accelerated cycle standing in for roughly two years of normal wear. It is what converts a laboratory result into a statement about the real service life of the piece.
Record producedPre-treatment noted on the test report
EN 1811:2023, release measurement
One week in artificial sweat, then measurement of the nickel released. Under the 2023 revision, sub-assemblies are separated or masked so each one is assessed in its own right, and where it is unclear whether the outer coating contains nickel the item is run both with and without pre-treatment.
Record producedMeasured result in µg/cm²/week per sub-assembly
Comparison against the limit
Against below 0.2 µg/cm²/week for pierced-part assemblies, or below 0.5 for other prolonged skin contact.
Record producedPass or fail against the stated limit, per sub-assembly
Scope
Which parts get assessed separately
One number for a whole earring is not a result. Under the 2023 revision each sub-assembly is assessed in its own right, which matters because the parts differ most exactly where it counts.
| Component | Applicable tier | Why it is assessed separately |
|---|---|---|
| Ear post | (a) below 0.2 | Enters the piercing channel and is the strictest exposure in the piece |
| Back plate / body | (b) or (c) below 0.5 | Rests against intact skin, usually with the fullest coating coverage |
| Ear nut / butterfly | (a) or (b) depending on construction | Often bought in rather than made in house, so it can differ in composition from the piece it fastens |
| Clasps and findings | (b) or (c) below 0.5 | Thinnest coating plus the most mechanical wear: the usual first failure point |
| Chain | (b) or (c) below 0.5 | Large surface area in continuous skin contact |
Evidence
Requesting a report
How to request a report
Tell us the base material and the finish color your styles use. Reports are issued per combination, so one report generally covers a whole group of styles. Requests go through the quote form with the material and finish stated.
Request a test reportLanguage
Why we do not say nickel free, or hypoallergenic
Both words are available to us and both would be easier to sell with. Here is why neither is ever used as a claim on this site.
What we say instead
Low nickel release, tested to EN 1811:2023 with EN 12472:2020 wear-and-corrosion pre-treatment, [result] µg/cm²/week, below the REACH Annex XVII entry 27 limit for [exposure category]. Report no. [number], [laboratory], [date]. Not a guarantee against all individual sensitivities.
Frequently asked questions
Does 316L stainless steel contain nickel?
Yes. 316L is an austenitic stainless steel and nickel is part of its composition. It is what makes the steel austenitic. Any supplier describing 316L jewelry as free of nickel is either mistaken about the material or hoping you are. The question that can be answered is how much nickel releases under skin contact, and that is measurable.
What is the difference between EN 1811 and EN 12472?
EN 1811:2023 is the measurement: the item sits in artificial sweat for a week and the released nickel is measured. EN 12472:2020 is the preparation that comes before it: an accelerated wear and corrosion cycle that simulates roughly two years of normal use. For a coated item the second one is what makes the first one meaningful, because it tests the coating in the state that wear will leave it in.
Why do ear posts have a different limit from the rest of the piece?
Because REACH Annex XVII entry 27 splits by exposure route. Paragraph (a) covers assemblies inserted into pierced ears and other pierced body parts, at below 0.2 µg/cm²/week. Paragraph (b) covers other items in prolonged skin contact, at below 0.5. Piercing exposes tissue rather than intact skin, which is why the limit is tighter.
Is a US brand bound by a European regulation?
Not directly. REACH is EU law. It appears here because US buyers use it as the available yardstick. There is no equivalent federal nickel release limit for adult jewelry, so a report against the EU method is the strongest comparable evidence on the table. It is also what you will need if the line ever ships into the EU or the UK.
Can I get the report for a specific style?
Reports are issued per material and finish combination rather than per SKU, because that is how the test works and how it is charged. One report typically covers every style sharing the same base material and the same coating. Ask for the combination your styles fall under and we will send the corresponding report.